title: "Do you need Rogers for RF?"
topic: "PCB materials"
answer: "Not at 2.4 GHz. A 3 cm trace on common FR-4 delivers 92% of its power there, against 96% on Rogers RO4350B. At 77 GHz the same trace delivers 21% on FR-4, so radar boards put one thin layer of Rogers on top."
url: "https://nearfieldnotes.com/notes/pcb-materials/"
site: "Near Field Notes"
author: "Michael Walker"
note: 30
family: "Board and fab"
published: "2026-11-11"
revised: "2026-11-11"
revision: 2
video: "https://nearfieldnotes.com/videos/pcb-materials/"
---

Note 30 · [Board and fab](https://nearfieldnotes.com/families/fab/) · Rev 2 · [Watch the video · 4:18](https://nearfieldnotes.com/videos/pcb-materials/)

PCB materials

# Do you need Rogers for RF?

**Short answer:** Not at 2.4 GHz. A 3 cm trace on common FR-4 delivers 92% of its power there, against 96% on Rogers RO4350B. At 77 GHz the same trace delivers 21% on FR-4, so radar boards put one thin layer of Rogers on top.

The wave is the signal along the trace at the frequency marked below. As the frequency climbs, more of it turns to heat in the FR-4 on the way.

RO4350B loses about a fifth as much in each cycle, so at 77 GHz 63% of its power arrives.

**Note 30’s opening figure: One trace, two materials.** 3 cm of 50 Ω microstrip, 2.4 to 77 GHz

![Note 30’s opening figure: One trace, two materials](https://nearfieldnotes.com/notes/pcb-materials/fig-opening.png)

*What the figure shows:* A 3 cm, 50 ohm trace on JLCPCB's common 4-layer stack, made once in FR-4 and once in RO4350B, as the frequency climbs from 2.4 to 77 GHz. At 2.4 GHz 92% of the power arrives on FR-4 and 96% on RO4350B. At 77 GHz the FR-4 trace's wave shrinks to under half its height by the end, and 21% arrives, against 63% on RO4350B. Below, the share that arrives at every frequency.

The same trace made in FR-4 and in RO4350B, each wave scaled to 1 where it starts. Below, the share of the power that arrives at each frequency, with the marked one drawn above.

**The numbers**

*Over the 3 cm trace. Each material at its own 50 Ω width, with the same copper.*

| Frequency | FR-4 loss | FR-4 arrives | RO4350B loss | RO4350B arrives |
|---|---|---|---|---|
| 2.4 GHz | 0.35 dB | 92% | 0.18 dB | 96% |
| 5 GHz | 0.62 dB | 87% | 0.29 dB | 94% |
| 10 GHz | 1.11 dB | 77% | 0.46 dB | 90% |
| 20 GHz | 2.02 dB | 63% | 0.73 dB | 85% |
| 28 GHz | 2.72 dB | 53% | 0.93 dB | 81% |
| 40 GHz | 3.76 dB | 42% | 1.20 dB | 76% |
| 60 GHz | 5.45 dB | 29% | 1.64 dB | 69% |
| 77 GHz | 6.86 dB | 21% | 1.98 dB | 63% |

## TI’s 77 GHz radar board

*AWR1642 evaluation board, 6 layers*

TI’s AWR1642 radar evaluation board answers the question with one thin sheet. Its radar chip, antennas and feeds sit on the top copper layer.

Each feed is a [50 Ω](https://nearfieldnotes.com/glossary/#g-characteristic-impedance) trace over the plane on layer 2. Between them is 0.10 mm of Rogers RO4835. Everything under layer 2 is FR-4.

**Fig. 30a: The radar board.**

![Fig. 30a: The radar board](https://nearfieldnotes.com/notes/pcb-materials/fig-30a.png)

*What the figure shows:* Figure 30a: TI's 77 GHz radar board, 45 by 35 mm, rendered from above. The radar chip sits at the left. Feeds run from it to two groups of antennas: short ones to the four receive antennas and longer ones to the transmit antennas. The longest feed, 30 mm, is drawn in blue. A notch cut from the corner shows the thin Rogers layer on top of the board.

Rendered from TI’s stack and layout notes, with the longest feed drawn in blue.

**The numbers**

| Part | What it is |
|---|---|
| Board | 45 × 35 mm, 1.43 mm thick, 6 layers |
| Top layer | Rogers RO4835 LoPro, 0.10 mm, between copper layers 1 and 2 |
| Layers 2 to 6 | FR-4: ITEQ IT-180A cores and 1080 prepreg |
| Feeds | 50 Ω microstrip on layer 1, 0.193 mm wide; the longest is 30 mm |
| Antennas | Four receive and three transmit columns of patches |

The Rogers is 7% of the board’s 1.43 mm. On that layer, a 3 cm feed delivers 56% of its power at 77 GHz.

That is less than the opening’s 63%. TI’s Rogers is 0.10 mm thick, half the 0.21 mm under the opening’s trace. A 50 Ω trace on it is 0.19 mm wide against 0.43 mm, and the narrower copper loses more: 0.51 dB/cm against 0.29.

Made in FR-4 prepreg of the same thickness, the same feed would deliver 21%. In RO3003, TI’s other choice for the top layer, 73%.

**Fig. 30b: Its stack, cut open.**

![Fig. 30b: Its stack, cut open](https://nearfieldnotes.com/notes/pcb-materials/fig-30b.png)

*What the figure shows:* Figure 30b: TI's radar board stack. Above, a corner of it rendered with its layers cut open. Below, the same stack drawn to scale, 1.43 mm in all: copper layer 1 with the feed's trace, 0.10 mm of RO4835, then copper layers 2 to 6 held apart by FR-4 prepreg and cores. The Rogers is 7% of the board's thickness.

Above, a corner of the board rendered with its layers cut. Below, the same stack to scale, both ways, with the feed’s trace on layer 1.

**The numbers**

*From TI’s SPRACG5, Figure 1, as processed. 1080 is the prepreg’s glass style.*

| Layer | Thickness | Metric |
|---|---|---|
| Copper L1 | 2.067 mil | 52.5 µm |
| RO4835 core | 4.000 mil | 101.6 µm |
| Copper L2 | 1.260 mil | 32.0 µm |
| IT-180A 1080 | 2.830 mil | 71.9 µm |
| IT-180A 1080 | 2.830 mil | 71.9 µm |
| Copper L3 | 1.260 mil | 32.0 µm |
| IT-180A core | 28.000 mil | 711.2 µm |
| Copper L4 | 1.260 mil | 32.0 µm |
| IT-180A 1080 | 2.691 mil | 68.4 µm |
| IT-180A 1080 | 2.691 mil | 68.4 µm |
| Copper L5 | 1.260 mil | 32.0 µm |
| IT-180A core | 4.000 mil | 101.6 µm |
| Copper L6 | 2.067 mil | 52.5 µm |
| **Total** | **56.22 mil** | **1428 µm** |

## What a board is made of

*Glass, resin and copper*

TI’s two materials are made the same way. A rigid board is glass cloth soaked in resin, with copper foil outside.

A core comes cured, with copper on both faces. Prepreg is the same cloth with its resin not yet cured. Pressed hot, it melts, glues the stack together and sets.

Change the resin and the glass, and four numbers change.

- **Dk.** How fast a signal travels, and how wide a 50 Ω trace is.
- **Df.** The share of each cycle that turns to heat.
- **Z-expansion.** How much the board swells when it is soldered.
- **Thermal conductivity, k.** How well it carries heat away.

**Fig. 30c: A board pulled apart.**

![Fig. 30c: A board pulled apart](https://nearfieldnotes.com/notes/pcb-materials/fig-30c.png)

*What the figure shows:* Figure 30c: a 4-layer board pulled apart into its five sheets: copper foil on top, a sheet of prepreg, the core with copper on both sides, a second sheet of prepreg and copper foil underneath. Pressed hot, the prepreg melts, glues the stack and sets.

The five sheets pressed into a 1.6 mm board, spread apart for the drawing and not to scale.

**The numbers**

*JLCPCB’s JLC04161H-7628 stack, 1.6 mm. Exploded for the drawing, not to scale.*

| Sheet | Thickness | What it is |
|---|---|---|
| Copper foil | 35 µm | The outer layers, etched after pressing |
| Prepreg | 0.2104 mm | Glass cloth in resin not yet cured, which glues the stack |
| Core | 1.0954 mm | Glass cloth in cured resin, copper on both sides: the inner layers |
| Prepreg | 0.2104 mm |  |
| Copper foil | 35 µm |  |

## Loss grows with frequency

*Df, and the field’s share*

Of those four numbers, Df sets the loss. The dielectric’s loss is its Df times the share of the field’s energy that runs through it, and it grows in step with frequency:

`α_d = 8.686 × (π f)/c √(ε_eff) q tanδ`

where α_d: loss per length in the dielectric (dB/m); f: frequency (Hz); c: speed of light (m/s); ε_eff: effective permittivity the wave sees (No unit); q: share of the field’s energy in the dielectric (No unit); tanδ: loss tangent, the datasheet’s Df (No unit).

`= 8.686 × (π × 77 GHz)/(3.00 × 10⁸ m/s) × √(3.19) × 0.874 × 0.018 = 197 dB/m = 1.97 dB/cm`

That is the opening’s FR-4 trace at 77 GHz. Its copper adds 0.32 dB/cm, for 2.29 dB/cm in all, so the dielectric takes 86% of the loss.

Copper’s part grows only with the square root of frequency. Over the 3 cm, decibels turn back into the share that arrives:

`P/P_0 = 10^(− α L /10)`

where P: power that arrives (W); P_0: power sent (W); α: loss per length, copper and dielectric (dB/cm); L: length of the trace (cm).

`= 10^(−2.29 dB/cm × 3 cm/10) = 21%`

Fig. 30d uses a third trace: 50 Ω on a 0.1 mm sheet, the thickness of the radar board’s top layer. It is made in seven materials, from the four families met one at a time further down.

At 10 GHz, 10 cm of it loses 3.9 dB on FR-4 and 1.3 dB on RO3003. At 77 GHz FR-4 loses 24.6 dB, and 0.3% arrives. Megtron 6 and RO4350B land side by side, 9.0 dB and 8.8 dB.

**Fig. 30d: The same trace on seven materials.**

![Fig. 30d: The same trace on seven materials](https://nearfieldnotes.com/notes/pcb-materials/fig-30d.png)

*What the figure shows:* Figure 30d: loss in 10 cm of the same 50 ohm trace on seven board materials, an open ring at 10 GHz and a dot at 77 GHz, each row in its family's color. FR-4: 3.9 dB at 10 GHz, 24.6 dB at 77 GHz. FR408HR: 2.5 dB at 10 GHz, 14.4 dB at 77 GHz. Megtron 6: 1.8 dB at 10 GHz, 9.0 dB at 77 GHz. RO4350B: 1.8 dB at 10 GHz, 8.8 dB at 77 GHz. Megtron 8: 1.4 dB at 10 GHz, 5.8 dB at 77 GHz. RO3003: 1.3 dB at 10 GHz, 5.6 dB at 77 GHz. RT/duroid 5880: 1.1 dB at 10 GHz, 4.8 dB at 77 GHz.

Loss in 10 cm of a 50 Ω trace on 0.1 mm, with the same copper on every material. The open ring is 10 GHz and the dot 77 GHz.

**The numbers**

*50 Ω microstrip on 0.1 mm, 1 oz rolled copper on every material, 10 cm long.*

| Material | Family | Dk | Df | 10 GHz | 77 GHz | Arrives at 77 GHz |
|---|---|---|---|---|---|---|
| FR-4 | FR-4 | 4.4 | 0.018 | 3.90 dB | 24.64 dB | 0% |
| FR408HR | Low-loss FR-4 grade | 3.65 | 0.0095 | 2.51 dB | 14.37 dB | 4% |
| Megtron 6 | Low-loss FR-4 grade | 3.61 | 0.004 | 1.81 dB | 8.99 dB | 13% |
| RO4350B | Hydrocarbon-ceramic | 3.66 | 0.0037 | 1.78 dB | 8.76 dB | 13% |
| Megtron 8 | Low-loss FR-4 grade | 3.08 | 0.0012 | 1.35 dB | 5.84 dB | 26% |
| RO3003 | PTFE | 3 | 0.001 | 1.31 dB | 5.59 dB | 28% |
| RT/duroid 5880 | PTFE | 2.2 | 0.0009 | 1.13 dB | 4.79 dB | 33% |

## The field stays in the top sheet

*Why one layer is enough*

A trace’s field runs from the trace to the copper plane under it. On TI’s board that plane is layer 2, 0.10 mm down, so the field crosses the Rogers and the air above and goes no further.

83% of its energy is in the RO4835 and 17% in the air. The layer 2 copper is 32 µm thick, many skin depths at 77 GHz, so none reaches the FR-4. The FR-4 under it only holds the board together.

**Fig. 30e: The radar trace’s field.**

![Fig. 30e: The radar trace’s field](https://nearfieldnotes.com/notes/pcb-materials/fig-30e.png)

*What the figure shows:* Figure 30e: TI's radar trace cut across, to scale, with the electric field's lines. The trace sits on 0.10 mm of RO4835 over the layer 2 copper plane. Most lines run straight down through the Rogers to the plane, and a few arc up through the air and come down beside the trace. None reach the FR-4 under the plane. 83% of the field's energy is in the RO4835 and 17% in the air.

Electric field lines from the 2D solve, crowded where the field is strong. To scale.

**The numbers**

*From the 2D solve of TI’s layer 1 trace, 0.193 mm wide on 0.1016 mm of RO4835, 50.1 Ω.*

| Where | Share of the field’s energy |
|---|---|
| In the RO4835 | 83.0% |
| In the air | 17.0% |
| Below the layer 2 plane | 0% |

## Heat moves the phase

*Dk against temperature*

Dk matters to a radar too. It drifts as a board warms, and the wave slows or speeds up with it. A long feed at a high frequency is many wavelengths long, so a small drift moves its phase a lot:

`Δφ = 360° × N × 1/2 s × TCDk × ΔT`

where Δφ: phase change at the feed’s end (degrees); N: wavelengths along the feed (No unit); s: share of a Dk change the wave feels (No unit); TCDk: dk change per degree (ppm/°C); ΔT: temperature swing (°C).

`= 360° × 22.6 × 1/2 × 0.86 × 200 ppm/°C × 125 °C = 87°`

That is a 5 cm length of Fig. 30d’s 0.1 mm trace on FR-4 at 77 GHz, warmed from −40 to 85 °C.

**Fig. 30f: Phase drift.**

![Fig. 30f: Phase drift](https://nearfieldnotes.com/notes/pcb-materials/fig-30f.png)

*What the figure shows:* Figure 30f: how far the phase at the end of a 5 cm feed moves at 77 GHz as the board warms from −40 to 85 °C. FR-4: 87.0 degrees. RO4350B: 20.0 degrees. RO3003: -1.1 degrees.

The phase at the end of a 5 cm, 50 Ω feed at 77 GHz on 0.1 mm, as in Fig. 30d, against the board’s temperature. RO3003’s is on 0.127 mm.

**The numbers**

*50 Ω microstrip at 77 GHz: FR-4 and RO4350B on 0.1 mm, RO3003 on 0.127 mm.*

| Material | TCDk | Wavelengths in 5 cm | Share of a Dk change felt | Phase change |
|---|---|---|---|---|
| FR-4 | +200 ppm/°C | 22.6 | 0.857 | 87.0° |
| RO4350B | +50 ppm/°C | 21.0 | 0.846 | 20.0° |
| RO3003 | −3 ppm/°C | 19.6 | 0.839 | −1.1° |

Phase drift

### 87° on FR-4, −1° on RO3003

**Field marks.** A 5 cm feed on Fig. 30d’s FR-4 is 22.6 wavelengths long at 77 GHz. From −40 to 85 °C its Dk climbs 2.5%, and its end’s phase moves 87°. On RO4350B it moves 20°, on RO3003 −1°.

**Look-alike.** Low loss read as low drift. RT/duroid 5880 has about RO3003’s Df, 0.0009 against 0.0010, but its Dk drifts −125 ppm/°C against −3.

**Range.** Rogers gives FR-4 a typical +200 ppm/°C and RO4350B +50. Higher-Dk RO3000 laminates drift far more: RO3010 is −395.

**Habitat.** Radars and phased arrays, whose feeds must stay in step. TI credits RO3003 with rolled copper for lower loss and better phase repeatability, and RO4835 for better yield.

## Heat leaving a part

*k, through the board*

Thermal conductivity, k, matters once a part runs hot. Heat from a part on top has to cross the board to reach a heatsink underneath. Each square centimeter of a layer holds it back by its thickness over its conductivity:

`R″ = t/k`

where R″: thermal resistance of a square centimeter of layer (°C·cm²/W); t: layer thickness (m); k: thermal conductivity (W/(m·K)).

`= (1.6 mm)/(0.4 W/(m·K)) = 40 °C·cm²/W against (76 µm)/(2.2 W/(m·K)) = 0.35 °C·cm²/W`

The first is plain 1.6 mm FR-4. The second is the thin dielectric of an aluminum IMS board, which sits on 1.5 mm of aluminum.

**Fig. 30g: One watt into an LED.**

![Fig. 30g: One watt into an LED](https://nearfieldnotes.com/notes/pcb-materials/fig-30g.png)

*What the figure shows:* Figure 30g: one watt into an LED's pad, on three boards cut through from the LED's center out to 10 mm, to scale, colored by how much hotter than the heatsink each point runs. FR-4, 1.6 mm: the pad runs 25.5 °C above the heatsink. FR-4 with 9 vias: the pad runs 11.4 °C above the heatsink. Aluminum IMS: the pad runs 2.8 °C above the heatsink.

Each board cut through from the LED’s center out to 10 mm, to scale, colored by how much hotter than the heatsink each point runs. The dark bar is the LED’s pad.

**The numbers**

*1 W into a 3 × 3 mm pad, a 1 oz pour 10 mm in radius, the board’s bottom on a heatsink held at 25 °C, no air cooling.*

| Board | Build | Pad above the heatsink |
|---|---|---|
| FR-4, 1.6 mm | 1.6 mm FR-4, k 0.4 W/m·K, 35 µm copper both sides | 25.5 °C |
| FR-4 with 9 vias | The same, with nine 0.3 mm plated vias under the pad | 11.4 °C |
| Aluminum IMS | 76 µm dielectric, k 2.2 W/m·K, on 1.5 mm aluminum, k 138 W/m·K | 2.8 °C |

Heat rise

### 25.5 °C hotter on FR-4, 2.8 °C on aluminum

**Field marks.** One watt into a 3 × 3 mm LED pad, the board on a heatsink. Through 1.6 mm of FR-4 the pad runs 25.5 °C hotter than the heatsink, with nine vias under it 11.4 °C, and on aluminum IMS 2.8 °C.

**Look-alike.** High Tg. Isola’s 370HR, Tg 180 °C, conducts the same 0.4 W/m·K as other FR-4.

**Range.** FR-4 conducts about 0.4 W/m·K and Bergquist’s HT-04503 IMS dielectric 2.2. Aluminum is 138, aluminum nitride 170 and copper 386.

**Habitat.** LED bulbs. Teardowns of GE’s and Cree’s A19 bulbs and the LIFX BR30 found aluminum boards. [Note 7](https://nearfieldnotes.com/notes/thermal-relief/) follows the same heat the other way, into a pad being soldered.

## Standard FR-4

*Glass-epoxy, on almost every board*

With the four numbers in hand, here are the families one at a time, starting with the board most people order. [Note 25](https://nearfieldnotes.com/notes/ufl-jumper/) follows the opening’s FR-4 trace at 5.5 GHz.

**Fig. 30h: FR-4 up close.**

![Fig. 30h: FR-4 up close](https://nearfieldnotes.com/notes/pcb-materials/fig-30h.png)

*What the figure shows:* Figure 30h: a close look at FR-4's makings, a few millimeters across. On the left, dry woven glass cloth, 2116 style. To the right the same cloth soaked in amber epoxy resin. On the resin, a sheet of copper foil with one corner peeled up.

Dry glass cloth on the left, the same cloth soaked in resin on the right, and copper foil on top. About 4 mm across.

**The numbers**

| Part | What it is |
|---|---|
| Glass cloth | 2116 style, as woven: yarns about 0.42 mm apart |
| Resin | Epoxy, flame-retardant |
| Copper foil | Electrodeposited, its rough side toward the resin to grip it |

Standard FR-4

### Df 0.018, $4 for five boards

**Field marks.** Nan Ya’s NP-155F, a JLCPCB 4-layer material, has a Df of 0.016 to 0.019 from 1 to 10 GHz. Shengyi’s S1141 swells 4.5% in thickness from 50 to 260 °C and delaminates after 2 minutes at 288 °C.

**Look-alike.** FR-4 read as one material. The name is a flame-retardant grade: Panasonic lists Megtron 4, Df 0.007 at 13 GHz, as FR-4.0 too.

**Range.** The opening’s 3 cm trace delivers 92% at 2.4 GHz, 77% at 10 GHz and 21% at 77 GHz.

**Habitat.** Almost every board, from JLCPCB’s default 2-layer Tg 135 FR-4 to OSH Park’s. [Note 3](https://nearfieldnotes.com/notes/antenna-ground/)’s 2.4 GHz antenna is etched on 1 mm of it.

## High-Tg and low-loss FR-4

*New resins, the same process*

Change only the resin and a board can take more soldering heat, or lose less. Fabs press these grades the way they press FR-4.

**Fig. 30i: A server-class board.**

![Fig. 30i: A server-class board](https://nearfieldnotes.com/notes/pcb-materials/fig-30i.png)

*What the figure shows:* Figure 30i: a 20-layer board, 165 by 105 mm and 3.2 mm thick, of the kind servers use, with a large processor package, rows of memory slots and an edge connector. Its cut edge shows the many thin layers.

A 20-layer board of the kind low-loss grades go into.

**The numbers**

*A render of the kind of board low-loss grades go into, not a particular product.*

| Part | What it is |
|---|---|
| Board | 165 × 105 mm, 3.2 mm thick |
| Layers | 20 copper layers, signal and ground in turn |

High-Tg and low-loss FR-4

### Df 0.025 down to 0.0012

**Field marks.** Isola’s high-Tg 370HR lasts 30 minutes at 288 °C and swells 2.8% from 50 to 260 °C. Low-loss Megtron 6 cuts Df to 0.004 at 10 GHz, Megtron 8 to 0.0012 at 14 GHz.

**Look-alike.** High Tg read as low loss. 370HR’s Tg is 180 °C, but its Df, 0.025 at 10 GHz, tops NP-155F’s, and its long-term rating is 130 °C.

**Range.** AMD’s cost table puts Megtron 6 at 3.5 times FR-4. Cisco measured 37% more loss on it at 10 GHz with standard foil than with smooth HVLP.

**Habitat.** Servers and routers. Panasonic called Megtron 6 “the standard of the high-end server router equipment material” in 2015.

## Hydrocarbon-ceramic

*Rogers RO4000*

The laminate most people mean by “Rogers” is ceramic-filled hydrocarbon, the first step up from FR-4 for RF.

**Fig. 30j: An RO4350B coupon.**

![Fig. 30j: An RO4350B coupon](https://nearfieldnotes.com/notes/pcb-materials/fig-30j.png)

*What the figure shows:* Figure 30j: a coupon of RO4350B, 0.76 mm thick, half of it still clad in copper and half etched back to the cream laminate, with a 50 ohm trace 1.67 mm wide across the bare half.

Half still clad in copper, half etched back to the laminate.

**The numbers**

| Part | What it is |
|---|---|
| Laminate | Rogers RO4350B, 0.030 in, design Dk 3.66 |
| Copper | 1 oz electrodeposited |
| Trace | 50 Ω microstrip, 1.67 mm wide |

Hydrocarbon-ceramic

### Df 0.0037, processed like FR-4

**Field marks.** RO4350B is ceramic-filled hydrocarbon on woven glass, with a Df of 0.0037 at 10 GHz and a design Dk of 3.66. Rogers says it runs through standard FR-4 processes with no sodium etch.

**Look-alike.** PTFE. “Rogers” often stands for any RF laminate, but Rogers calls RO4000 “reinforced hydrocarbon/ceramic laminates – not PTFE”.

**Range.** At JLCPCB five boards cost 46.5 times as much as in FR-4, but at retail the laminate costs about 4 times: €147.15 per square foot for 60 mil RO4003C against €35.60 for 1.57 mm FR-4. Its filler wears out drills in 2,000 to 3,000 hits.

**Habitat.** The top layer of TI’s radar board, as RO4835, the same laminate made to resist oxidation.

## PTFE

*The lowest loss, and soft*

For the lowest loss and the steadiest Dk, boards go to PTFE, the plastic in Teflon, filled with ceramic or glass.

**Fig. 30k: An RO3003 coupon.**

![Fig. 30k: An RO3003 coupon](https://nearfieldnotes.com/notes/pcb-materials/fig-30k.png)

*What the figure shows:* Figure 30k: a coupon of RO3003, 0.76 mm thick, half clad in copper and half bare, with a 50 ohm trace 1.92 mm wide across the bare half, wider than on RO4350B because RO3003's Dk is lower.

The same coupon as Fig. 30j, in ceramic-filled PTFE with rolled copper. Its lower Dk makes the 50 Ω trace wider.

**The numbers**

| Part | What it is |
|---|---|
| Laminate | Rogers RO3003, ceramic-filled PTFE, 0.030 in, Dk 3.00 |
| Copper | 1 oz rolled |
| Trace | 50 Ω microstrip, 1.92 mm wide |

PTFE

### Df 0.0010, Dk steady with heat

**Field marks.** RO3003 has a Df of 0.0010 at 10 GHz, and its Dk drifts only −3 ppm/°C. On the opening’s trace at 77 GHz, 3 cm of it delivers 78%.

**Look-alike.** RT/duroid 5880. It is PTFE too, with glass microfiber, but it swells 237 ppm per degree in thickness against RO3003’s 25.

**Range.** Rogers’ fab guide calls these laminates soft and asks for support through scrubbing. RO4003C is about 18 times as stiff as 5880. Before plating, the hole walls need plasma or a sodium etch.

**Habitat.** 77 GHz car radar. Rogers sells RO3003 for it, and teardowns of Bosch’s mid-range radar and Autoliv’s 77 GHz radar found hybrid PTFE and FR-4 boards.

## Polyimide flex

*No glass, so it bends*

Leave out the glass and a board can bend. Flex circuits are thin polyimide film with copper on it.

**Fig. 30l: A rigid-flex board, folded.**

![Fig. 30l: A rigid-flex board, folded](https://nearfieldnotes.com/notes/pcb-materials/fig-30l.png)

*What the figure shows:* Figure 30l: a rigid-flex board folded in half. Two green FR-4 boards carrying parts are joined by a strip of amber polyimide flex, bent through 180 degrees so one board sits over the other.

Two FR-4 boards joined by polyimide flex, folded so one sits over the other.

**The numbers**

| Part | What it is |
|---|---|
| Rigid | FR-4 1.0 mm, green mask |
| Flex | polyimide 50 um core, 18 um copper, 37 um coverlay |
| Fold | 12 mm wide, 16 mm free between the boards |

Polyimide flex

### Bends, and takes up water

**Field marks.** DuPont’s Pyralux AP is polyimide with no adhesive layer. Its Df is 0.003 at 10 GHz, and DuPont rates it for 6,000 flex cycles. It takes up 0.8% water.

**Look-alike.** LCP. Liquid crystal polymer bends too, with lower loss: Rogers gave its ULTRALAM 3850HT a Df of 0.0020 at 10 GHz. Murata builds its mmWave 5G antenna modules on its own LCP board.

**Range.** Five 2-layer flex boards, 0.11 mm thick, cost $16.00 at JLCPCB. Würth’s rigid-flex rules give a bend radius of 10 times the flex’s thickness for two copper layers.

**Habitat.** Cables inside phones and cameras, and rigid-flex boards that fold into tight cases: FR-4 where the parts sit, polyimide where it bends.

## Aluminum IMS

*Insulated metal substrate*

When the job is heat, the base can be metal. An IMS board is one copper layer on a thin dielectric on aluminum.

**Fig. 30m: An LED bulb’s board.**

![Fig. 30m: An LED bulb’s board](https://nearfieldnotes.com/notes/pcb-materials/fig-30m.png)

*What the figure shows:* Figure 30m: an LED bulb's round aluminum board, 40 mm across, with eight LEDs on a ring. A notch cut in its edge shows the 76 µm dielectric under the copper and the 1.5 mm of aluminum under that.

The notch in the edge shows the layers.

**The numbers**

| Part | What it is |
|---|---|
| Board | 40 mm across |
| Base | 1.5 mm aluminum |
| Dielectric | 76 µm, as Bergquist HT-04503 |
| Copper | 35 µm |
| LEDs | Eight 2835 (2.8 x 3.5 x 0.75 mm) |

Aluminum IMS

### k 2.2, against FR-4’s 0.4

**Field marks.** A filled polymer dielectric between the copper and an aluminum base. Bergquist’s HT-04503 is 76 µm thick at 2.2 W/m·K, on aluminum at 138. In Fig. 30g it holds a 1 W LED to 2.8 °C above the heatsink.

**Look-alike.** A board that conducts like metal. The aluminum under it conducts 63 times better than the dielectric, so the dielectric’s thickness and k are what to read a datasheet for.

**Range.** JLCPCB offers aluminum only as a 1-layer board, with what it calls a “1W” dielectric. Five cost $4.00, the same promotional price as FR-4.

**Habitat.** LED bulbs and lamps, and power parts that sit on a heatsink.

## Ceramic

*Copper bonded to ceramic*

For hundreds of watts, power modules bond thick copper straight onto a ceramic sheet.

**Fig. 30n: A power module’s substrate.**

![Fig. 30n: A power module’s substrate](https://nearfieldnotes.com/notes/pcb-materials/fig-30n.png)

*What the figure shows:* Figure 30n: a half-bridge power module's substrate: copper islands bonded to a thin silicon nitride sheet, with two silicon carbide transistor dies and their aluminum bond wires.

A half bridge: two transistor dies on copper islands, bonded to silicon nitride.

**The numbers**

| Part | What it is |
|---|---|
| Ceramic | Si3N4 AMB 40 x 30 x 0.32 mm |
| Copper | 0.3 mm |
| Dies | SiC MOSFET 4.6 x 4.0 x 0.18 mm, sintered |
| Wires | Al 380 um source, 125 um gate |

Ceramic

### Up to 170 W/m·K, and brittle

**Field marks.** Copper 0.127 to 0.8 mm thick, bonded to a ceramic sheet. Rogers’ curamik line rates silicon nitride at 90 W/m·K and aluminum nitride at 170, against 24 for alumina.

**Look-alike.** IMS. Both carry hot parts, but an IMS board insulates with 76 µm of polymer at 2.2 W/m·K, and a ceramic substrate with a sheet at 24 to 170.

**Range.** Ceramics are brittle: CoorsTek gives its aluminas a fracture toughness of 4 to 5 MPa·m½.

**Habitat.** Power modules in EV traction inverters. onsemi lists a silicon nitride isolator in its EliteSiC traction module, and Rogers sells its silicon nitride substrates for traction inverters.

## What five boards cost

*One fab, one day*

Price is why boards mix materials. Fig. 30o lines up one fab’s price for five 100 × 100 mm boards in each material, from $4.00 in FR-4 to $186.13 in RO4350B.

FR-4’s and aluminum’s $4.00 are promotions, so the ratios say more about the price list than the laminates. Copper core is the IMS build with a copper base in place of aluminum.

**Fig. 30o: What five boards cost, by material.**

![Fig. 30o: What five boards cost, by material](https://nearfieldnotes.com/notes/pcb-materials/fig-30o.png)

*What the figure shows:* Figure 30o: what five 100 by 100 mm boards cost at JLCPCB on 6 November 2026, by material. FR-4: $4.00. Aluminum IMS: $4.00. High-Tg FR-4: $11.12. Polyimide flex: $16.00. Copper core: $50.00. PTFE: $71.13. RO4350B: $186.13.

JLCPCB’s web prices on 6 November 2026, before shipping. Bars in color are the families of Fig. 30d, and outlined bars the boards outside them. The builds differ in thickness and layers, and the numbers give each one.

**The numbers**

*JLCPCB’s web prices, 6 November 2026, before shipping. The FR-4 and aluminum prices are promotional. The PTFE and RO4350B quotes include the ENIG finish they require.*

| Material | Build | Five boards | Against FR-4 |
|---|---|---|---|
| FR-4 | 1.6 mm, 2 layers | $4.00 | 1.0× |
| Aluminum IMS | 1.6 mm, 1 layer | $4.00 | 1.0× |
| High-Tg FR-4 | KB6165F, 1.6 mm, 2 layers | $11.12 | 2.8× |
| Polyimide flex | 0.11 mm, 2 layers | $16.00 | 4.0× |
| Copper core | 1.6 mm, 1 layer | $50.00 | 12.5× |
| PTFE | ZYF300CA-C, 0.76 mm, 2 layers | $71.13 | 17.8× |
| RO4350B | 1.52 mm, 2 layers | $186.13 | 46.5× |

## Mixing materials in one board

*Hybrid stackups*

A hybrid puts the costly laminate only where the field runs. On TI’s radar board that is one sheet on top, because a microstrip’s field ends at the plane under it, as Fig. 30e shows.

A stripline is different. It runs between two planes, so its field fills the layers above and below it. With Megtron 6 on one side and FR-4 on the other, the loss lands about halfway: 14.4 dB over 10 inches at 16 GHz, against 19.9 dB all FR-4 and 7.9 dB all Megtron 6.

**Fig. 30p: A stripline between two materials.**

![Fig. 30p: A stripline between two materials](https://nearfieldnotes.com/notes/pcb-materials/fig-30p.png)

*What the figure shows:* Figure 30p: a stripline cut across, to scale: a trace between two copper planes, with 0.13 mm of Megtron 6 core below it and 0.15 mm of FR-4 prepreg above. Its field lines run both up and down. 57% of the field's energy is in the FR-4 and 43% in the Megtron 6.

Field lines from the 2D solve, to scale. The trace sits on the Megtron 6 core, with FR-4 prepreg pressed over it.

**The numbers**

*50 Ω stripline, 0.113 mm wide, 18 µm copper.*

| Where | Share of the field’s energy |
|---|---|
| FR-4 prepreg above, and beside the trace | 56.9% |
| Megtron 6 core below | 43.1% |

**Fig. 30q: Loss in the stripline.**

![Fig. 30q: Loss in the stripline](https://nearfieldnotes.com/notes/pcb-materials/fig-30q.png)

*What the figure shows:* Figure 30q: loss over 10 inches of 50 ohm stripline at 16 GHz, three ways. All FR-4: 19.9 dB. Megtron 6 core, FR-4 prepreg: 14.4 dB. All Megtron 6: 7.9 dB.

The same 50 Ω stripline, three ways, 10 inches long at 16 GHz. The two-tone bar is the mixed build, its FR-4 prepreg drawn over its Megtron 6 core.

**The numbers**

*10 in of 50 Ω stripline: 0.13 mm core below, 0.15 mm prepreg above, 18 µm copper with smooth HVLP foil.*

| Build | 16 GHz | Arrives | 28 GHz | Arrives |
|---|---|---|---|---|
| All FR-4 | 19.9 dB | 1% | 32.9 dB | 0% |
| Megtron 6 core, FR-4 prepreg | 14.4 dB | 4% | 23.4 dB | 0% |
| All Megtron 6 | 7.9 dB | 16% | 12.2 dB | 6% |

Hybrids come with rules, and the fab sets most of them.

- **Keep the stack balanced.** IPC-6012 allows 0.75% bow and twist on a board with surface-mount parts, and its automotive addendum leaves unbalanced builds to agreement between buyer and maker. TI’s board has a 4 mil core at each face: RO4835 at the top, FR-4 at the bottom.
- **Bond at FR-4’s temperatures.** Fusion-bonding PTFE takes 371 °C or more, past the 345 °C where IT-180A FR-4 starts to break down. So PTFE hybrids are glued with prepreg or bondply that cures at 175 to 250 °C.
- **Mind the swelling.** From 50 to 260 °C, IT-180A swells 2.7% in thickness and RO4350B about 0.67%. The plated holes through both have to take the difference.
- **Ask the fab first.** Each material drills and cleans its holes its own way. Rush PCB notes that each mix needs its own UL approval, and that a hybrid only pays when about three quarters of the thickness is the cheaper material.

**Fig. 30r: What each bond needs.**

![Fig. 30r: What each bond needs](https://nearfieldnotes.com/notes/pcb-materials/fig-30r.png)

*What the figure shows:* Figure 30r: the temperatures a hybrid's bonds need, against the point where FR-4 starts to break down. RO4450F bondply: 175 °C. FR-4 prepreg cure: 182–185 °C. SpeedWave prepreg: 200 °C. 2929 bondply: 245–250 °C. FR-4 starts to break down: 345 °C. PTFE fusion bond: 371 °C.

The temperature each bonding step needs, against the 5% weight loss point of IT-180A FR-4.

**The numbers**

*From Rogers’ processing guides for RO4450F, SpeedWave 300P, 2929 and PTFE fusion, Isola’s 370HR guide for the FR-4 cure, and ITEQ’s IT-180A sheet for 5% weight loss.*

| Step | Temperature |
|---|---|
| RO4450F bondply | 175 °C |
| FR-4 prepreg cure | 182–185 °C |
| SpeedWave prepreg | 200 °C |
| 2929 bondply | 245–250 °C |
| FR-4 starts to break down | 345 °C |
| PTFE fusion bond | 371 °C |

## Choosing a material

*Heat, bending and loss*

Start from what the board has to do. Most boards end at FR-4, and the rest add a costly material only where it pays.

Key to board materials

### Which material does my board need?

1. 1a A part on it must shed watts through the board Go to 6
2. 1b No part runs that hot Go to 2
3. 2a The board has to bend or fold Polyimide flex
4. 2b It stays flat Go to 3
5. 3a On FR-4 a trace loses more than the link can spare Go to 4
6. 3b It can spare the loss FR-4
7. 4a Fast digital links run on many layers Low-loss FR-4 grade
8. 4b RF runs on one or two layers Go to 5
9. 5a It needs the lowest loss and a phase that holds with heat PTFE on those layers
10. 5b Low loss is enough Hydrocarbon on those layers
11. 6a A few watts from LEDs or a regulator Aluminum IMS
12. 6b Hundreds of watts from power switches Ceramic

TI’s radar board in Fig. 30a ends at 5b: RO4835 on layer 1 and FR-4 under it. Bosch’s and Autoliv’s radars, built with PTFE and FR-4, end at 5a.

## Pick a material yourself

*Seven materials, 1 to 77 GHz*

Choose a frequency and a length for the opening’s trace. Each bar is the share of the power that arrives, with the trace made in that material at its own 50 Ω width.

At 2.4 GHz over 3 cm, every material delivers 92% or more. At 77 GHz they spread from 21% to 82%.

**Note 30’s explorer: Power that arrives, by material.**

![Note 30’s explorer: Power that arrives, by material](https://nearfieldnotes.com/notes/pcb-materials/fig-explore.png)

*What the figure shows:* The share of the power that arrives along the chosen length of the opening's trace at the chosen frequency, for each of seven board materials, from FR-4 at the top to RT/duroid 5880 at the bottom.

The opening’s trace, 0.21 mm over its plane, with the same copper on every material.

**The numbers**

*Each material at its own 50 Ω width over 0.21 mm, with the same copper.*

| Over 3 cm | FR-4 | FR408HR | Megtron 6 | RO4350B | Megtron 8 | RO3003 | RT/duroid 5880 |
|---|---|---|---|---|---|---|---|
| 1 GHz | 96% | 97% | 98% | 98% | 98% | 98% | 98% |
| 2.4 GHz | 92% | 95% | 96% | 96% | 97% | 97% | 97% |
| 5 GHz | 87% | 91% | 93% | 94% | 95% | 95% | 96% |
| 10 GHz | 77% | 85% | 90% | 90% | 93% | 93% | 94% |
| 16 GHz | 68% | 80% | 86% | 87% | 91% | 91% | 92% |
| 28 GHz | 53% | 70% | 80% | 81% | 87% | 88% | 89% |
| 40 GHz | 42% | 62% | 75% | 76% | 84% | 85% | 87% |
| 60 GHz | 29% | 50% | 68% | 69% | 80% | 81% | 84% |
| 77 GHz | 21% | 42% | 62% | 63% | 77% | 78% | 82% |

#### Conditions

- **Opening trace:** 50 Ω microstrip on JLCPCB’s JLC04161H-7628 stack: 0.2104 mm of prepreg over the layer 2 plane, 1 oz standard electrodeposited copper, Sq 3.2 µm, no solder mask. In FR-4, Dk 4.4 and Df 0.018, it is 0.37 mm wide. In RO4350B, at its design Dk of 3.66 and Df 0.0037, 0.43 mm. The explorer puts all seven materials on this trace. 2.4 GHz is taken at 2.45 GHz.
- **Fig. 30d:** 50 Ω microstrip on 0.1 mm, 1 oz rolled copper, Sq 0.4 µm, the same on every material.
- **Radar trace:** TI’s layer 1: 4 mil RO4835 LoPro at its process Dk of 3.48 and Df 0.0037, 2.067 mil copper with LoPro foil, Sq 0.9 µm, 0.19 mm wide. The FR-4 swap is 4 mil of IT-180A 1080 prepreg at Dk 3.7 and Df 0.018, with standard foil. The RO3003 swap is 5 mil, with rolled copper.
- **Materials:** Dk and Df at 10 GHz from each datasheet: FR408HR 3.65 and 0.0095, Megtron 6 3.61 and 0.004, RO4350B 3.66 and 0.0037, RO3003 3.00 and 0.0010, RT/duroid 5880 2.20 and 0.0009. Megtron 8, 3.08 and 0.0012, is Panasonic’s 14 GHz figure. FR-4 is a typical 4.4 and 0.018, inside NP-155F’s Df range.
- **Loss:** A 2D field solve of each cross-section. The dielectric loses its share of the field’s energy times its Df, as in the formula above. Copper loss comes from incremental inductance, with the Hammerstad roughness model. Df is held at its datasheet value at every frequency. Against Rogers’ measured 1.3 dB per inch for 5 mil RO3003G2 at 77 GHz, the solve gives 1.28.
- **Stripline:** 50 Ω between two planes: 0.13 mm core below, 0.15 mm prepreg above, 18 µm copper with HVLP foil.
- **Phase:** Each material’s TCDk from its datasheet, with FR-4 at Rogers’ typical +200 ppm/°C. The 2D solve gives how much of a Dk change the wave feels. FR-4 and RO4350B on 0.1 mm, RO3003 on 0.127 mm.
- **Heat:** Steady heat conduction in a disc 15 mm in radius: 1 W into a pad with the area of 3 × 3 mm, a 1 oz copper pour 10 mm in radius, and the bottom held at 25 °C. FR-4 at 0.4 W/m·K. The vias count as 2.2% copper under the pad. The IMS is 76 µm at 2.2 W/m·K on 1.5 mm of aluminum at 138.
- **Video:** The video’s 92% at 2.4 GHz and 21% at 77 GHz came from two traces, a 2.4 GHz board’s on JLCPCB’s 4-layer stack and TI’s layer 1 made in FR-4. The opening sweeps the first alone, which gives the same two numbers.
- **Renders:** Blender, from the stacks and builds named in each figure’s numbers.

Simulated only. Nothing on this page has been measured on a board yet.

#### Limits

- Real Df creeps up with frequency, so the 77 GHz losses favor FR-4 if anything.
- No solder mask, bends or vias. In a hybrid, vias run through both materials, and [Note 17](https://nearfieldnotes.com/notes/via-stubs/) covers what their stubs cost.
- Radiation and surface waves aren’t counted.
- The phase drift is a straight-line estimate from each TCDk. Rogers’ measured curves bend.
- The heat runs have a perfect heatsink and no air, so only the boards differ.
- Prices are one fab on one day, and FR-4’s and aluminum’s are promotional.

#### Files

- sim/xsec.py The 2D field solve: impedance, field shares and loss of a trace in any layered stack
- sim/loss.py Fig. 30d’s seven materials, TI’s radar trace and its swaps, the phase drift and the striplines
- sim/site.py The opening’s trace from 2.4 to 80 GHz, the explorer’s seven materials, and the field lines
- sim/thermal.py The 1 W LED on three boards
- sim/materials.py Each material’s Dk and Df and each copper foil’s roughness, with sources
- render/stack.py The radar board, its stack and the 4-layer board pulled apart
- render/parts.py The weave, the coupons, the server board, the rigid-flex, the LED board and the power module

#### Sources

- [TI, SPRACG5, mmWave radar sensor RF PCB design guide, the AWR1642 board’s stack](https://www.ti.com/lit/pdf/spracg5)
- [Rogers, RO4000 data sheet, RO4350B and RO4003C](https://www.rogerscorp.com/-/media/project/rogerscorp/documents/advanced-electronics-solutions/english/data-sheets/ro4000-laminates-ro4003c-and-ro4350b---data-sheet.pdf)
- [Rogers, RO4835 data sheet](https://www.rogerscorp.com/-/media/project/rogerscorp/documents/advanced-electronics-solutions/english/data-sheets/ro4835-laminate-data-sheet.pdf)
- [Rogers, RO3000 data sheet, RO3003 and RO3010](https://www.rogerscorp.com/-/media/project/rogerscorp/documents/advanced-electronics-solutions/english/data-sheets/ro3000-laminate-data-sheet-ro3003----ro3006----ro3010----ro3035.pdf)
- [Rogers, RT/duroid 5880 data sheet](https://www.rogerscorp.com/-/media/project/rogerscorp/documents/advanced-electronics-solutions/english/data-sheets/rt-duroid-5870---5880-data-sheet.pdf)
- [Rogers, copper foils for high frequency materials, each foil’s Sq](https://www.rogerscorp.com/-/media/project/rogerscorp/documents/advanced-electronics-solutions/english/properties---detailed-characteristics/copper-foils-for-high-frequency-circuit-materials.pdf)
- [Rogers, RT/duroid fabrication guidelines, soft laminates and hole-wall prep](https://www.rogerscorp.com/-/media/project/rogerscorp/documents/advanced-electronics-solutions/english/fabrication-information/fabrication-guidelines-rt-duroid-5880lz-high-frequency-laminates.pdf)
- [Rogers ROG Blog, epoxy versus high frequency laminates, epoxy’s typical TCDk](https://microwavejournal.com/blogs/1-rog-blog/post/16662-fr-4-versus-high-frequency-laminates)
- [Rogers, RO3003G2 launch, its 1.3 dB per inch at 77 GHz](https://www.microwavejournal.com/articles/31678-rogers-launches-next-generation-laminates-for-automotive-radar-sensor-applications)
- [Microwave Journal, Rogers ULTRALAM 3850HT launch, its Df](https://www.microwavejournal.com/articles/23897-rogers-high-temp-lcp-laminates-improves-construction-of-multilayer-circuit-boards)
- [Rogers, curamik ceramic substrates, each ceramic’s k and copper](https://www.rogerscorp.com/-/media/project/rogerscorp/documents/advanced-electronics-solutions/english/product-information/curamik-ceramic-substrates-product-information-and-data-sheet.pdf)
- [Rogers, curamik Performance Plus, silicon nitride for traction inverters](https://www.rogerscorp.com/advanced-electronics-solutions/curamik-ceramic-substrates/curamik-performance-plus)
- [Rogers, RO4000 circuit processing guidelines, standard processes and drill life](https://www.rogerscorp.com/-/media/project/rogerscorp/documents/advanced-electronics-solutions/english/fabrication-information/fabrication-guidelines-ro4000-series-ro4003cro4350bro4835-laminates.pdf)
- [Rogers, RO4400 bonding layers processing guidelines, RO4450F’s cure](https://www.rogerscorp.com/-/media/project/rogerscorp/documents/advanced-electronics-solutions/english/fabrication-information/fabrication-guidelines-ro4400-bonding-layers.pdf)
- [Rogers, SpeedWave 300P processing guidelines, its cure](https://rogerscorp.com/-/media/project/rogerscorp/documents/advanced-electronics-solutions/english/fabrication-information/fabrication-guidelines-speedwave-300p-prepreg.pdf)
- [Rogers, 2929 bondply processing guidelines, its bond temperature](https://www.rogerscorp.com/-/media/project/rogerscorp/documents/advanced-electronics-solutions/english/fabrication-information/2929-bondply-multi-layer-board-processing-guidelines.pdf)
- [Rogers ROG Blog, fusion bonding, its 371 °C](https://www.microwavejournal.com/blogs/1-rog-blog/post/20670-fusion-bonding-forms-reliable-multilayer-circuits)
- [Nan Ya, NP-155F family data sheet, its Df](https://www.eurocircuits.com/content/uploads/2024/05/NP-155FTL_NP-155FR_NP-155FB.pdf)
- [Shengyi, S1141 data sheet, its z-expansion and T288](https://www.ipcb.com/public/upload/file/20200928/f9e114d6592941eb23cd1b00875ad64b.pdf)
- [Isola, 370HR data sheet, its Tg, Df, k and long-term rating](https://www.isola-group.com/wp-content/uploads/data-sheets/370hr-laminate-prepreg.pdf)
- [Isola, FR408HR data sheet](https://www.isola-group.com/wp-content/uploads/data-sheets/fr408hr-laminate-and-prepreg.pdf)
- [Isola, prepreg processing guide, epoxy prepreg’s cure](https://www.isola-group.com/wp-content/uploads/370HR-Laminate-and-Prepreg-Processing-Guide052020.pdf)
- [ITEQ, IT-180A data sheet, its 345 °C and 2.7%, from a distributor’s copy](https://a-contract.ru/fileadmin/datasheets/base-material/IT-180A.pdf)
- [Panasonic, Megtron 6 data sheet](https://api.pim.na.industrial.panasonic.com/file_stream/main/fileversion/244768)
- [Panasonic, circuit board materials catalog, Megtron 4 to 8](https://api.pim.na.industrial.panasonic.com/file_stream/main/fileversion/251291)
- [Panasonic, Megtron models, Megtron 8’s Dk and Df](https://industrial.panasonic.com/ww/products/pt/megtron/models)
- [Panasonic, Megtron 4 data sheet, its flame-retardant grade, from a distributor’s copy](https://a-contract.ru/fileadmin/datasheets/base-material/R5725-Megtron-4.pdf)
- [I-Connect007, interview with Panasonic, 2015, Megtron 6 as the standard](https://iconnect007.com/article/88806/panasonic-meeting-market-needs-with-higherperformance-megtron-7/88809/design)
- [AMD, UG863, material properties and relative cost](https://docs.amd.com/r/en-US/ug863-versal-pcb-design/Material-Properties-and-Insertion-Losses)
- [Hinaga and others, Cisco and Missouri S&T, copper roughness and loss on Megtron 6](https://www.electronics.org/system/files/technical_resource/E8%26S20_02.pdf)
- [DuPont, Pyralux AP data sheet, from Insulectro](https://insulectro.com/wp-content/uploads/2025/04/Pyralux-AP-Laminate-Data-Sheet-2-25.pdf)
- [Würth Elektronik, rigid-flex design rules, the bend radius](https://www.we-online.com/files/pdf1/design-rules-rigidflex-2f-xri-cbt-en.pdf)
- [Murata, mmWave 5G antenna module on its MetroCirc LCP board](https://www.murata.com/en-us/news/connectivitymodule/mmwave-rf/2021/1013)
- [Bergquist, Thermal Clad HT-04503 data sheet, from a fab’s copy](https://www.mclpcb.com/wp-content/uploads/2021/05/BergquistHT-04503.pdf)
- [Ventec, VT-4B3 data sheet, aluminum’s and copper’s k, from a fab’s copy](https://www.mclpcb.com/wp-content/uploads/2021/05/Ventec-200518VT-4B3.pdf)
- [CoorsTek, advanced alumina, its fracture toughness](https://www.coorstek.com/media/4235/advanced-alumina.pdf)
- [onsemi, NVXR17S90M2SPC EliteSiC traction module](https://www.onsemi.com/products/discrete-power-modules/power-modules/silicon-carbide-sic-modules/nvxr17s90m2spc)
- [Hackaday, LED bulb teardowns, GE and Cree](https://hackaday.com/2019/02/05/what-happened-to-the-100000-hour-led-bulbs)
- [iFixit, LIFX BR30 teardown](https://www.ifixit.com/Teardown/LIFX+BR30+Teardown/153277)
- [Research and Markets, Bosch mid-range radar teardown, 2015](https://prnewswire.co.uk/news-releases/bosch-mid-range-radar-mrr-sensor---reverse-costing-analysis-539383801.html)
- [Research and Markets, Autoliv 77 GHz radar teardown, 2017](https://www.prnewswire.co.uk/news-releases/teardown-analysis-of-autolivs-77ghz-multi-mode-radar-spc-with-a-comparison-with-the-bosch-mrr-and-delphi-racam---research-and-markets-616430494.html)
- [Eurocircuits, bow and twist, quoting IPC-6012’s 0.75%](https://www.eurocircuits.com/warp-twist/)
- [IPC-6012EA, automotive addendum, unbalanced construction](https://www.ipc.org/TOC/IPC-6012EA_TOC.pdf)
- [Rush PCB in PCD&F, balancing stackups, when a hybrid pays and its UL approval](https://pcdandf.com/pcdesign/index.php/editorial/menu-features/18331-balancing-stackups-and-circuitry)
- [JLCPCB, instant quote, read 6 November 2026](https://cart.jlcpcb.com/quote)
- [RF-Microwave, laminate prices, RO4003C](https://www.rf-microwave.com/en/rf-microwave-laminates/371/)
- [Digi-Key, MG Chemicals 555 glass-epoxy sheet](https://www.digikey.de/en/products/detail/mg-chemicals/555/559707)
- [OSH Park, services](https://docs.oshpark.com/services/)

What should the next note be? [Ask for one](https://nearfieldnotes.com/#ask-for-a-note)

---

Source: https://nearfieldnotes.com/notes/pcb-materials/

Cite as: Michael Walker, “PCB materials”, Near Field Notes, Note 30, Rev 2, 11 Nov 2026. https://nearfieldnotes.com/notes/pcb-materials/

Figures: free to reuse under CC BY 4.0 (https://nearfieldnotes.com/license/). Each one's image is linked under its name. Credit Michael Walker, Near Field Notes, and link the figure: this address plus #fig- and its number, like https://nearfieldnotes.com/notes/pcb-materials/#fig-30a.